Polyvel Anti-Static Concentrate VSE10 Effects in LDPE Cast Film
Anti-static concentrate for blown film electronic packaging applications
Static Decay Test
Static Decay Time (seconds)*
Level of VS-E10
Day 7
Day 16
Day 27
Day 35
Day 56
Day 65
Day 84
2.5%
0.30
0.28
0.32
0.36
0.46
0.48
0.48
3.0%
0.26
0.25
0.28
0.30
0.40
0.42
0.42
Surface Resistivity Test
Surface Resistivity**
Level of VS-E10
Day 7
Day 16
Day 27
Day 35
Day 56
Day 65
Day 84
2.5%
1.3 x10"
1.4 x10"
1.5 x10"
1.8 x10"
1.8 x10"
1.9 x10"
1.9 x10"
3.0%
1.3 x10"
1.2 x10"
1.2 x10"
1.4 x10"
1.4 x10"
1.6 x10"
1.6 x10"
*Federal Test Method 4046 (Mil. Spec. B-81705C) <2.0 sec., decay from 5 kv to 0 kv at 12% relative humidity
**ASM D257-78, Surface Resistivity <10E12 (Ohms per square)